Clear Coat Disaster...


Author
Message
fibernoob
fibernoob
Supreme Being (334 reputation)Supreme Being (334 reputation)Supreme Being (334 reputation)Supreme Being (334 reputation)Supreme Being (334 reputation)Supreme Being (334 reputation)Supreme Being (334 reputation)Supreme Being (334 reputation)Supreme Being (334 reputation)
Group: Forum Members
Posts: 34, Visits: 134
Hi all.

After some attempts I have successfully made a resin infused part and learn t the hard way with the many costly mistakes.

However I am having great difficulty with the clear coat stage.

The clear coat seems to just open many holes and give a nasty irregular (big orange peel like) finishing and has damaged all my attempts.

I had initially suspected it to be release agent in the part expelling the clear coat since the first part came out with a matt finish (due to excessive and unpolished release agent).

During the next attempts I used less release agent and polished the mold thoroughly leaving it with high gloss finish.

The part seemed to come out OK  … but since the part will be exposed to sunlight I opted to get it clear coated.

I also thought it would give the part more depth and a higher quality look and avoid yellowing in future.

We have tried various clear coating methods but it always just opens up many holes again and again…

Has anyone experienced this before ? Help would be greatly appreciated.

  • Method : Resin Infusion Process
  • Resin : Huntsman High Viscosity Epoxy Resin
  • Release agent : Huntsman Renlease QZ5111
  • Clearcoat : Automive PU Clear / PPG ACS



Attachments
IMG_8804.jpg (1.2K views, 59.00 KB)
Reply
fibernoob
fibernoob
Supreme Being (334 reputation)Supreme Being (334 reputation)Supreme Being (334 reputation)Supreme Being (334 reputation)Supreme Being (334 reputation)Supreme Being (334 reputation)Supreme Being (334 reputation)Supreme Being (334 reputation)Supreme Being (334 reputation)
Group: Forum Members
Posts: 34, Visits: 134
Sure ... it also didn’t add up.

I changed the clear as a last resort since I had redone all the rest.



Before applying to the carbon we tested on metal and interestingly enough the one that least stuck do the carbon had a better result on metal and vice-Versa.

On pure resin (left over from infusion) both stuck perfectly. So I then blamed the release agent.

To make sure ..... I made a quick sheet and added both wax based and pvc release agent to test.(possible release agent in the fiber opening clear)


The newer clear seemed to perform better again.

My only guess would be possible better chemical compatibility between them ...


Thanks for the reply ... I will keep testing.

GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Threaded View
Threaded View
fibernoob - 9 Years Ago
Interloper393 - 9 Years Ago
fibernoob - 9 Years Ago
Interloper393 - 9 Years Ago
Hanaldo - 9 Years Ago
MarkMK - 9 Years Ago
fibernoob - 9 Years Ago
             What brNd did you use?
Interloper393 - 9 Years Ago
                 Sherwin Williams 2k automotive clear
fibernoob - 9 Years Ago
Hanaldo - 9 Years Ago
fibernoob - 9 Years Ago