Hi all.

After some attempts I have successfully made a resin infused part and learn t the hard way with the many costly mistakes.

However I am having great difficulty with the clear coat stage.

The clear coat seems to just open many holes and give a nasty irregular (big orange peel like) finishing and has damaged all my attempts.

I had initially suspected it to be release agent in the part expelling the clear coat since the first part came out with a matt finish (due to excessive and unpolished release agent).

During the next attempts I used less release agent and polished the mold thoroughly leaving it with high gloss finish.

The part seemed to come out OK  … but since the part will be exposed to sunlight I opted to get it clear coated.

I also thought it would give the part more depth and a higher quality look and avoid yellowing in future.

We have tried various clear coating methods but it always just opens up many holes again and again…

Has anyone experienced this before ? Help would be greatly appreciated.

  • Method : Resin Infusion Process
  • Resin : Huntsman High Viscosity Epoxy Resin
  • Release agent : Huntsman Renlease QZ5111
  • Clearcoat : Automive PU Clear / PPG ACS



Attachments
IMG_8804.jpg (1K views, 59.00 KB)
Reply
MarkMK
MarkMK
Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)
Group: Forum Members
Posts: 338, Visits: 2K

Additionally, it sounds like your clear-coat is fish-eyeing...is this what you mean by it 'opening-up' which might suggest that there's some reaction with whatever you're cleaning the part with

If there's a suitable product available where you are, you might have better success using an in-mould coating prior to making your parts where the spraying technique required isn't quite so critical


GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Threaded View
Threaded View
fibernoob - 8 Years Ago
Interloper393 - 8 Years Ago
fibernoob - 8 Years Ago
Interloper393 - 8 Years Ago
Hanaldo - 8 Years Ago
MarkMK - 8 Years Ago
fibernoob - 8 Years Ago
             What brNd did you use?
Interloper393 - 8 Years Ago
                 Sherwin Williams 2k automotive clear
fibernoob - 8 Years Ago
Hanaldo - 8 Years Ago
fibernoob - 8 Years Ago

Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search