Hi, it´s happened to me twice already. I make a carbon fiber sheet and on the surface there are pores and micro pores. I do it with a glass, once with weight making a sandwich with another glass behind and again, without weight and without glass behind. Both pores have come out Crying



Something else happens to me, too. To cut the CF I use Dremel with disc to cut plastic. If I don´t make the cuts fast, due to the heat of the cut, along the cut the epoxy resin remains as curved, to the sides of the cut Sad

Any advice?

Regards.
Replies
Hanaldo
Hanaldo
Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)
Group: Forum Members
Posts: 2.5K, Visits: 28K
Be aware that the 'wet-lay' technique you are using to make the sheets will quite often come out with some pinholes on the surface, it takes some practice to get a cosmetically perfect wet-laid piece. 

Also when trimming, it sounds like you are cutting too close to the size that you want. High rpm cutting tools like Dremels and angle grinders will create a lot of heat, which can cause the resin to delaminate from the fibres and leave you with a fuzzy edge. It is best to cut slightly over-size, say about 1mm, and then sand the edge back to the exact size that you require. Finishing with 320 grit or higher will give you a nice smooth edge that won't give you nasty splinters! 
M. Martin
M. Martin
Junior Member (24 reputation)Junior Member (24 reputation)Junior Member (24 reputation)Junior Member (24 reputation)Junior Member (24 reputation)Junior Member (24 reputation)Junior Member (24 reputation)Junior Member (24 reputation)Junior Member (24 reputation)
Group: Forum Members
Posts: 4, Visits: 43
Thanks for your tips! Later on will try to make the leaves of CF by resin infusion, but for now for economy i do it hand layup.
I take note of all your advices!
Thank you very much!
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...





Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search