Newbie problem casting water clear sphere


Author
Message
SC
SC
SC
posted 10 Years Ago HOT
Junior Member (17 reputation)Junior Member (17 reputation)Junior Member (17 reputation)Junior Member (17 reputation)Junior Member (17 reputation)Junior Member (17 reputation)Junior Member (17 reputation)Junior Member (17 reputation)Junior Member (17 reputation)
Group: Forum Members
Posts: 1, Visits: 5
Hi,

I'm a newbie to using resin, and have started a little 'shed' project in order to give me a few minutes to escape the long list of housework assignments Smile

My ultimate goal is to cast some water clear resin spheres to encapsulate various organic items (flowers, etc). I've experimented making some molds (one part and two parts) out of Addition Cure Silicone. These all appear to be fine.
http://s33.postimg.org/fyg7z6wi7/silicone_Mold.jpg

When I attempt to cast Water Clear Resin in them, the end result always  comes out partially covered in unpleasant surface ridge lines (see photo's). With my amateur eye, it appears that as the resin cures and shrinks, the partially set surface peels away from the mold at various places, leaving little contact trails.
http://s33.postimg.org/jpka50mxb/sphere2.jpg

http://s33.postimg.org/nexekkwsv/sphere1.jpg

I've experimented with different catalyst mix ratios from 0.2% to 5%, with no success yet.

What am I doing wrong? Wrong material, bad technique, environmental factors...?

Any help would be appreciated, as my lovely and patient wife will soon start asking me some awkward questions...

Thanks,
Simon
Zebra
Zebra
Supreme Being (190 reputation)Supreme Being (190 reputation)Supreme Being (190 reputation)Supreme Being (190 reputation)Supreme Being (190 reputation)Supreme Being (190 reputation)Supreme Being (190 reputation)Supreme Being (190 reputation)Supreme Being (190 reputation)
Group: Forum Members
Posts: 14, Visits: 32
Are you using exactly the right resin to hardener ratio? Odd surface features can appear when too much hardener is used by sometime trying to speed up the process or attempting the project without a gram scale. 

I have also seen odd surface marks from working in a place that's too humid, too hot, not hot enough. Also from not degassing a resin that needed it (as some of my clear urethanes do). Can also be the pattern of the mold release.

If none of these apply then you can try a different clear resin or a different mold. Or, just sand off the marks and repolish until it goes clear again.
Fasta
Fasta
Supreme Being (6.7K reputation)Supreme Being (6.7K reputation)Supreme Being (6.7K reputation)Supreme Being (6.7K reputation)Supreme Being (6.7K reputation)Supreme Being (6.7K reputation)Supreme Being (6.7K reputation)Supreme Being (6.7K reputation)Supreme Being (6.7K reputation)
Group: Forum Members
Posts: 468, Visits: 3.5K
Just try another brand material or different type of material.

Maybe a polyurethane resin?




Warren (Staff)
Warren (Staff)
Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)
Group: Administrators
Posts: 2.5K, Visits: 8.5K
How long are you leaving the part prior to demoulding?  We have seen similar effects when items are released too soon from the mould. Also what sort of size is the sphere? It may well be getting quite hot as the resin cures off and be borderline exotherming if the volume is quite large.

Warren Penalver
Easy Composites / Carbon Mods - Technical Support Assistant
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search