Davidpetty1988
Davidpetty1988
posted 9 Years Ago
ANSWER
HOT
Topic Details
Group: Forum Members
Posts: 26,
Visits: 89
Just having a little trouble perfecting my resin infusion only my second attempt. can anyone help I think its degassing related but not 100% I have tiny gaps in the resin around the fibres only on the mould finish side none on the peel ply side. I assume this is air. Any ideas??
Dave
Tags
degass
Gaps
resin
Edited
9 Years Ago by
Davidpetty1988
Reply
Like
6
Replies
Davidpetty1988
Davidpetty1988
posted 9 Years Ago
ANSWER
HOT
Post Details
Group: Forum Members
Posts: 26,
Visits: 89
Just being reading a thread is it because I'm clamping the resin line first and I should actually be clamping the vac line first?? Any threads or topics I should check out?
Edited
9 Years Ago by
Davidpetty1988
Reply
Like
6
Matt (Staff)
Matt (Staff)
posted 9 Years Ago
ANSWER
HOT
Post Details
Group: Forum Members
Posts: 680,
Visits: 1.9K
Hi David,
There can be a number of causes of pin-holes like this but I'd say that 99% of the time it can be prevented by allowing the laminate to be a little more resin-rich. When a pin-hole free finish is a priority (as opposed to ultimate lightness being the #1 priority) then follow this sequence for pin-hole free perfection:
1. Allow a good few seconds of 'flushing' resin through the laminate when the laminate is fully infused and resin is making its way down the resin line (unless you have a peel-ply resin break in place, in which case let the resin crawl through that for a minute or so).
2. Clamp off the vacuum line.
3. Wait a little while (vague I know but it depends on the size of what you're infusing: small parts, 10-20 secs, large parts, up to a minute or two).
4. Clamp off the resin line.
This sequence goes against logic slightly for an infusion but what it does is allow a little extra resin into the laminate, probably decreasing the fibre fraction from 60:40 to maybe 58:42. This subtle amount of surplus resin does wonders for the pin holes you're experiencing and is these steps are pretty-much standard for the professional infusion guys we supply.
I hope this helps; let us all know if it does!
Matt
Matt Statham
Easy Composites / Carbon Mods - Technical Sales
Tags
clamp
infusion
pin hole
surface finish
Reply
Like
11
GO
Merge Selected
Merge into selected topic...
Merge into merge target...
Merge into a specific topic ID...
Open Merge
Threaded View
Threaded View
Trouble with perfect finish
Davidpetty1988
-
9 Years Ago
Just being reading a thread is it because I'm clamping the resin line first and I should actually be...
Davidpetty1988
-
9 Years Ago
Hi David, There can be a number of causes of pin-holes like this but I'd say that 99% of the time...
Matt (Staff)
-
9 Years Ago
Post Reply
Like
6
Similar Topics
Post Quoted Reply
Reading This Topic
Login
Login
Remember Me
Reset Password
Resend Validation Email
Login
Facebook
Google
Explore
Messages
Mentions
Search