I am having a problem with GC50 and shrinkage.
I've noticed shrinkage before in sharp right -angled corners, where the gelcoat has pulled away and out from the corner, often following one surface or the other leaving a void one side. Sometimes a bigger void one side and a smaller the other.

This time I have seen a fairly large shrinkage, shown below. I gave a thicker than normal coat of Sprayed GC50, with 15% white Polyester pigment, 3% styrene 2.5% MEKP
This piece is scrap obviously, and I've had to strip it out and start again.

I am using a gravity fed spraygun, with a 1.8mm nozzle. It's not a gel coat specific gun but does the job for me as the part is not huge. I would have thought that the gel coat gun would have provided a thicker layer anyway?

The mould is very well seasoned now, and I use TR regular wax only.

Any thoughts? This is probably the one problem I have with GC50, in all other aspects it suits me perfectly. I'd like to get on top of this, otherwise it's back yet agin to finding a epoxy compatible poletser gel coat!

http://www.talkcomposites.com/Uploads/Images/5cd8e7ce-57fe-4ee9-92f6-c347.jpg
Replies
Warren (Staff)
Warren (Staff)
Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)
Group: Administrators
Posts: 2.5K, Visits: 8.5K
If the coat is too thick or the MEKP is too high for the temperature, then greater shrinkage than you would expect is a possibility.  It can be common in corners where there is a higher likelihood of a thicker coating being applied.  The hotter it gets during cure, the more likely it will shrink significantly.

Warren Penalver
Easy Composites / Carbon Mods - Technical Support Assistant
alex.mc
alex.mc
Supreme Being (121 reputation)Supreme Being (121 reputation)Supreme Being (121 reputation)Supreme Being (121 reputation)Supreme Being (121 reputation)Supreme Being (121 reputation)Supreme Being (121 reputation)Supreme Being (121 reputation)Supreme Being (121 reputation)
Group: Forum Members
Posts: 18, Visits: 52
Temperature was 23/25c, mostly 25c as I have a low-bake oven/warming cabinet that's thermostat controlled and pretty accurate.

Humidity I don't know, but maybe 60% at a guess?

I have always tended to use 2.5% MEKP

What's the minimum percentage of MEKP that would still kick to a cure? Has anyone any experience of using lesser amounts?

I have redone the moulds this morning using a little more styrene, 5% and the 2% MEKP so will see what the result is.
I've also put some tape on the back of the mould where it delaminated, and sprayed over that edge to try and create a "Tie-down" effect.

Another question on this subject of GC50.......
What's the scenario of multiple coats of GC50 to create depth? For example, I spray a coat on, then leave it for 3/4 hours and then spray another layer on top?