Group: Forum Members
Posts: 592,
Visits: 1.9K
|
The few pieces I have done in alu honeycomb so far have been done with the smallest cell version from EC, cut down to 3 and 5 mm thickness.
They are bonded with the EC Permabond stuff for Alu honeycomb.
This thin alu honeycomb cornforms very easily to compound curves. The nomex stuff less so.
Compared to test pieces in nomex honeycomb, the Nomex is slightly heavier, and does not permanently distort as easily as the alu.
On the alu version of the test-panel an 80 kg/ sq cm pressure test left a permanent 1 mm deformation, but the Nomex version using ordinary laminating resin as bonding did not permanently deform at the same pressure.
When the alu-honeycomb version failed it cracked completely, and at what seemed like a lower impact level.
I would think that in an impact scenario the Nomex wins... but you can make the alu versin thicker for the same weight and that will make it stiffer.
"Sapere Aude"... Dare to KNOW!
The written word is the only truly efficient vehicle for transmitting a complex concept from mind to mind...
103% of all people do not understand statistics...
Do not adjust our mind, theres a fault in reality :-)
|