I'm suddenly interesting in how tubes are made.  If I needed to make a tube with an accurate 80mm ID how would I go about it?  Its all fairly new to me so please type slowly and with small words!  The tube needs to bear around 1-1.5 bar of pressure so in my head I was considering an 80mm wax cylinder and roll wrapping some UD around it then putting some braided sleeve over the top and bagging the whole lot.  Its the only way I could tink to do it.

Tube would form the outer case for a wren jet turbine.
Hanaldo
Hanaldo
Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)
Group: Forum Members
Posts: 2.5K, Visits: 28K
80mm is 3", but this is how I built my 4" pipe:

http://www.talkcomposites.com/10433/4-intake-pipe

The method would work for yours. 
asmasm
asmasm
Supreme Being (97 reputation)Supreme Being (97 reputation)Supreme Being (97 reputation)Supreme Being (97 reputation)Supreme Being (97 reputation)Supreme Being (97 reputation)Supreme Being (97 reputation)Supreme Being (97 reputation)Supreme Being (97 reputation)
Group: Forum Members
Posts: 15, Visits: 189
For straight tubing solarcomposites sells inexpensive sleeves and silicone coated heat shrink tubing. Then you just need a section of tubing with and outer diameter matching your desired inner diameter. I used 1 layer of parchment paper as a release material and the carbon tube slid right off.
FLD
FLD
Supreme Being (3.7K reputation)Supreme Being (3.7K reputation)Supreme Being (3.7K reputation)Supreme Being (3.7K reputation)Supreme Being (3.7K reputation)Supreme Being (3.7K reputation)Supreme Being (3.7K reputation)Supreme Being (3.7K reputation)Supreme Being (3.7K reputation)
Group: Forum Members
Posts: 468, Visits: 2.7K
It's just the one I need and it'd need to be in high temp resin.  I think the tube / prachment / sleeve is the way forwards.