I have had a few request for details showing how I do a project from start to finish so here goes.Smile

Some of you may have gathered from some of my posts that I hate skinning, I have huge admiration for anyone who manages to make a living from doing it as I certainly can't. So when I was asked by a customer to skin the door mirrors from his Fiesta ST my initial reaction was "no thank you". After mulling things over I thought maybe there is another approach to this, make skins that can be made with infusion and then bonded on afterwards. As there seems to be lots of Fiestas out there and Fords kindly fit the same mirrors to all the models there could be a potential market for something that could be DIY fitted without the customer having to remove the covers, send them for skinning and have the car off the road until they came back. So here is how it was done.

First the original covers where removed from the car and given a degrease and a good coat of PVA.

Then I wet laid three layers of 200grm onto them. This was followed by flatting, re coating, flatting re coating until a smooth high gloss finish was achieved. ( this is why I hate skinning ) The final skins would be 2 layers plus roughly 0.2 gap for bonding them on.

These skins where then trimmed and released from the originals.

Because I wanted to produce two new skins at a time the two new skins where fixed to some Kingspan to form a pattern to mould form. The whole pattern was then given a layer of coating resin with some black pigment added and polished. ( black shows up any imperfections/scratches).

Because of the shape of the skins this would have to be a split mould, so the pattern was cut down the middle and a flange added. The whole thing was then bonded to a base board and any gaps filled with filleting wax.

A mould was then made using Uni Mould. The two halves where then bolted together with some gum tape between the flanges.

GC50 was then sprayed into the mould for UV protection.

The mould was then laid up with two layers of 200grm and bagged ready for infusion.

Once infused and cured they were trimmed using the originals as a template and given a polish.

If they prove popular then I think pre-preg may be the way forward to reduce manufacturing times and increase profit.


Warren

Carbon Copies Ltd
Edited 11 Years Ago by wozza
Replies
wozza
wozza
Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)
Group: Forum Members
Posts: 688, Visits: 5.4K
Here you go CraigSmile

Carbon Copies Ltd
Matthieu Libeert
Matthieu Libeert
Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)
Group: Forum Members
Posts: 955, Visits: 3.4K
Thanks for sharing! looks great!

Matthieu Libeert
Founder MAT2 Composites X Sports
website:
www.mat2composites.com




Atomant
Atomant
Forum Member (45 reputation)Forum Member (45 reputation)Forum Member (45 reputation)Forum Member (45 reputation)Forum Member (45 reputation)Forum Member (45 reputation)Forum Member (45 reputation)Forum Member (45 reputation)Forum Member (45 reputation)
Group: Forum Members
Posts: 7, Visits: 694
Warren they look great. Has given me some idea how that spoiler of mine could be done. When you say it had to be a split mould is that because the shape sort of curves over itself? and is there any flex in a finished part when you pull it from the mould? 

Also what do you use for cutting down the mould - a slitting disc in a dremel?

G
wozza
wozza
Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)
Group: Forum Members
Posts: 688, Visits: 5.4K
Atomant (05/03/2014)
Warren they look great. Has given me some idea how that spoiler of mine could be done. When you say it had to be a split mould is that because the shape sort of curves over itself? and is there any flex in a finished part when you pull it from the mould? 

Also what do you use for cutting down the mould - a slitting disc in a dremel?

G


Hi, yes the sides curve under creating an undercut. If I had made individual moulds then they would have released ok but because I wanted to produce the parts in pairs I would have had to destroy the pattern to release it from the mould. The parts themselves would have probably released ok with a bit of flexing the problem being that because they are only 2 layers thick you run the risk of cracking the part. Also on thin parts it is easy to damage them when removing the peel ply and flow mesh, this way the parts are locked into the mould making it easier to remove before demoulding if that makes sense.
On small parts like this I use a Dremel with the supplied slitting disks, on large parts the angry grinder comes out, again with a slitting disk fittedSmile

Warren

Carbon Copies Ltd
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Threaded View
Threaded View
wozza - 11 Years Ago
Brian2fast - 11 Years Ago
wozza - 11 Years Ago
wozza - 11 Years Ago
             Thanks for sharing! looks great!
matthieutje65 - 11 Years Ago
Atomant - 11 Years Ago
wozza - 11 Years Ago
FLD - 11 Years Ago
Warren (Staff) - 11 Years Ago
FLD - 11 Years Ago
wozza - 11 Years Ago
Warren (Staff) - 11 Years Ago
Bonobo - 11 Years Ago
wozza - 11 Years Ago
tha_pop - 11 Years Ago
     Thanks
Bonobo - 11 Years Ago

Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search