By Leew - 6/2/2013 1:48:58 PM
Just found out that there are apparently some incompatabilities with epoxy and polyester resin and that one cannot be laid over the other and visa versa. Is that true? I made a part with epoxy and then used some polyester body filler on it before putting some more epoxy in it which has not cured properly, I was wondering, could the body filler have affected the epoxy?
|
By wozza - 6/2/2013 10:23:46 PM
Probably the Styrene in the Body Filler being drawn out by the application of the Epoxy. Most Body Fillers need sealing especially if "freshly" applied and still green.
|
|