By aumlee - 3/8/2013 11:30:05 PM

Hello,

I am having issues getting my gel coat to cure. I am using easy composites clear gel coat with a black pigment and catalyst. The left over gel coat in the mixing beaker is curing after around an hour, however the gel on the mould is not curing. The first time I left it for 24 hours before deciding to start again. The second time I added more catalyst and has been around 5 hours and is still wet. It is in a cold workshop. Any help would be appreciated.
Thank you
By aumlee - 3/11/2013 11:30:29 AM

Thanks for your help. I think the sub 6°c workshop was the issue.

·