By Paulfr - 2/20/2021 8:51:52 AM
Hi,
I make carbon fiber fins for freediving with OOA prepreg twill 200 gsm I use a mold and a counter mold in press and a heating system under the mold
The issue I am having: Sometimes my part comes out curved lengthwise instead of being perfectly flat.
If anyone has an idea of to solve this issue it will help me a lot.
Thanks
|
By Paulfr1 - 2/27/2021 6:17:06 PM
Hi, The mold was hotter on the ends than in the middle. I changed the position of the heating elements.
The parts are now perfectly flat :-)