+xYour root cause is that the laminate is slightly lean. Try leaving the resin feed open for another minute or two after closing the vacuum outlet to eliminate surface porosity like this.
Then sanding the surface before painting can also open up porosity if you haven't got enough resin to sand into before hitting the fibres. For this reason, I believe it is better to not sand the surface before clearing. Instead, clean the surface very well with isopropyl alcohol or a paint prep solvent, and then use a grey or gold 3M scuff pad to key the surface without actually removing any resin.
For issues like you are having currently, it is actually possible to fill the pinholes in one application if you are using a premium quality high solids clear. It requires really loading it up, so you need to let each coat dry to the touch before you spray the next coat to avoid runs and solvent pop. It can often take as many as 6 or 7 coats, so it can take a few hours. And the clear may sink back into the pinholes when it cures, which usually isn't that noticeable but if it bugs you then just flat back and polish or spray a final coat.
Awesome thank you hanaldo, i see exactly what you mean by it being lean and ill give that a go on my next infusion, for my paint i used PPG so its good stuff, i am still learning all this, so ill try your paint procedure and see how i go, i was trying to fill the holes after 2 coats, clearly ive been worrying to much ๐, and i have been lightly sanding, ill go to the shops and buy scuff pad ๐