By mmcqui - 7/9/2020 5:47:48 PM
Hi there
Looking for some advice, poured my resin one week ago on a grouted bottle top table, apart from a couple of small bubbles, I was fairly happy with for a first attempt at resin.
I went to give the table a wipe down last night and on drying it I noticed that there appears to be a film after cleaning, especially on the outer of the table. I’m fairly sure it was ok before cleaning but I am absolutely sure it wasn’t there a couple days ago.
Do I need to sand down and pour again or will polishing help this, I’m pretty gutted as it looked great. It still looks shiny at a distance but under direct light and up close it’s not great.
I have tried to wipe with just water and it clears until dry.
Any help would be appreciated
Matthew
|
By SleepingAwake - 7/11/2020 10:37:23 AM
I would assume it is amine blush due to improper mixing. Can be polished out...
|
|