By jp233 - 2/6/2018 2:12:07 PM
Hi all,
I’m trying to infuse a new spinacker pole for my dinghy from a mandrel.
Mandrel is 3000mm long, thick end is 150mm dia and thin end is 50mm dia.
Layup is 200g weave 300g uni X4 200g weave.
The previous one didnt go well so I’m asking for some of your input.
The last one we did the weave and all the uni in one hit leaving the top wave for a seperate one. We used peel ply coiled helicularly, then bread wrap with the easy flow mesh over that, two spiral coils (One for in, one for out places onnoposite sides of the pole) then the bag.
Resin in was at the fat end that fed in to the spiral plugged at the other end with some breater The out pipe was fed into the out spiral, again with the breather over.
Used infusion resin, 10mm tubes with 6mm spiral.
Problems: it took forever for the resin to compleate the infusions, when we unwrapped, there were dry patches.
Has anyone got some hints as to how to improve his process?
If you need more info please say, will try to add photos when I find them.
Thanks Jamie
|
By polaraligned - 2/7/2018 8:25:01 PM
Can you use Soric 2mm core? It will act both as a core for rigidity and a flow medium. Put it between the 4 layers of uni.
|
|