inside of Mould edge not getting any resin
http://www.talkcomposites.com/Topic20961.aspx
By Davo456
-
4/4/2016 8:13:31 PM
The simple Z shaped piece (see photo) I've tried to do by resin infusion, but both the internal and exterior bends are resin starved.
mould is simple 3 bits of plastic, so nothing complex.
Would I be better doing this be wet layup and vacuum afterwards, rather than infusion ?
By davro
-
4/5/2016 10:37:59 AM
Agreed it looks like a small amount of bridging occurred, the product looks like it's slightly resin lean.
Close the output line first and keep the input line feeding resin to make it a little more resin rich.
Keep on infusing