By Dogger - 5/26/2015 2:48:50 PM

Hi folks.

i have a car which a previous owner painted matt black, its not my choice, but it is a race car so spending a lot having it resprayed is a waste as it won't make it go any faster!

i want to mould the panels as spares, but in carbon, and hopefully replace all the panels with home-made carbon ones eventually, but can i take moulds from something that is painted with a matt paint or will it adversely affect the surface of the mould and will it tend to have more bite- so it won't release cleanly?

thanks
By Hanaldo - 5/27/2015 12:40:57 PM

Yep, PVA is your friend. Spray it on like it's a paint, get a nice thick application. You won't have any issues. If the paint is a really bad job then it may come off the part and stay in the mould, but as long as you've got PVA it'll come off with a quick blast with a high pressure washer.