		| By davro - 9/30/2014 9:22:00 PM 
 Hi,
 
 I finally got around to creating a mould for 1/10 scale touring car, so I thought I would share with you helpful people
  
 I had a brand new body shell left over from me racing days.
 This new body shell was the perfect candidate to take a mould from, and I also had quite a bit of Easy Composites Uni Mould System left over from a previous project
 
 So I had all the necessary goodies to create a 1/10 body shell mould!
 
 And some spare time to make a mould and video with some royalty free music, good times
  Here is a video showing the making of the mould.Easy Leased the table 2 coatsEasy Leased the body shell 3 coats Uni-Mould Tooling Gelcoat 3 medium coats Uni-Mould Coupling Coat (100g Chopped Strand Mat)Uni-Mould Tooling Resin (450g Chopped Strand Mat)Lots of gloves and plastic cups
 
 
 
  
  
  
  
  
  
  
  
  
  
   |  
		| By davro - 10/19/2014 6:37:43 PM 
 Stickers on and Clear Coat applied
  
 ) Finish spoiler
 ) Sand back with 3000 grit
 ) Polish
 
 Pleased with having the stickers under the clear coat gives a nice effect
  
 
 
  
  
  
  
  
  
  
  
  
   |  |