Layers of jute composites for 3 mm thick sheet.
http://www.talkcomposites.com/Topic10254.aspx
By rbpatil
-
3/14/2014 5:17:35 PM
How many layers of Biotex jute fibre plain weave 290 g are to be used for making of epoxy matrix composite sheets of 3 mm thickness by compression moulding process?
By tack talk
-
4/24/2014 10:52:34 PM
I would use 8 layers assuming the following
Biotex Flax density = 1.46g/cm3
Epoxy resin density = 1.20g/cm3
Laminate has 43% rw