Eg160 Mould - Hairline Cracks after heat cycle


Author
Message
bennyT
b
Supreme Being (169 reputation)Supreme Being (169 reputation)Supreme Being (169 reputation)Supreme Being (169 reputation)Supreme Being (169 reputation)Supreme Being (169 reputation)Supreme Being (169 reputation)Supreme Being (169 reputation)Supreme Being (169 reputation)
Group: Forum Members
Posts: 11, Visits: 777
Hey all,

I have been using EG160 tooling gel coat for my moulds backed up with carbon fibre and EL160 for items being made with ooa prepreg.

On a couple of occasions after the first attempt at making a part and after the heat cycle I have noticed hairline cracking in the gelcoat (see attached picture).

Note: I have only ever seen this after the heat cycle and releasing the part. Before the heat cycle everything is fine. 

Any ideas?
Edited 5 Years Ago by bennyT
Warren (Staff)
Warren (Staff)
Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)
Group: Administrators
Posts: 2.5K, Visits: 8.5K
I would check the thickness of your gel and also stability of the mould.  If the gel is too thick and/or the mould moves quite a bit during curing etc then it could cause issues.

Also I see a bit of print, perhaps check you leave it long enough to cure before demoulding as that can cause print as well as making it harder to demould, which may make cracks that become visible later in the cure cycle.

Warren Penalver
Easy Composites / Carbon Mods - Technical Support Assistant
bennyT
b
Supreme Being (169 reputation)Supreme Being (169 reputation)Supreme Being (169 reputation)Supreme Being (169 reputation)Supreme Being (169 reputation)Supreme Being (169 reputation)Supreme Being (169 reputation)Supreme Being (169 reputation)Supreme Being (169 reputation)
Group: Forum Members
Posts: 11, Visits: 777
Warren (Staff) - 9/22/2021 4:11:02 PM
I would check the thickness of your gel and also stability of the mould.  If the gel is too thick and/or the mould moves quite a bit during curing etc then it could cause issues.

Also I see a bit of print, perhaps check you leave it long enough to cure before demoulding as that can cause print as well as making it harder to demould, which may make cracks that become visible later in the cure cycle.

Hey Warren, 

With stability in mind, I laminated the mould with 2x200g carbon followed by 3x600g carbon. Given the stiffness of carbon and the shape of this mould, in your opinion should this be enough to give good stability?

Warren (Staff)
Warren (Staff)
Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)
Group: Administrators
Posts: 2.5K, Visits: 8.5K
Sounds like it should be plenty stiff. Perhaps too thick gel or demoulding too soon? 

Warren Penalver
Easy Composites / Carbon Mods - Technical Support Assistant
bennyT
b
Supreme Being (169 reputation)Supreme Being (169 reputation)Supreme Being (169 reputation)Supreme Being (169 reputation)Supreme Being (169 reputation)Supreme Being (169 reputation)Supreme Being (169 reputation)Supreme Being (169 reputation)Supreme Being (169 reputation)
Group: Forum Members
Posts: 11, Visits: 777
Warren (Staff) - 9/23/2021 12:29:51 PM
Sounds like it should be plenty stiff. Perhaps too thick gel or demoulding too soon? 

Ok thanks, will give it a try 👍