oekmont - 6/12/2020 9:21:50 AM
When you do infusion, full vacuum is important. Otherwise there would be trapped air in every corner, because the resin would overflow the corner, leaving behind a cavity of 50% pressurised air. During the process the cavity will shrink down to half it's size while it reaches atmospheric pressure. Accordingly a 100% vacuum cavity shrinks down to zero size.
And you should remember that rotary vane pumps were not invented for composite use only, especially not for vacuum bagging. Many applications require a high vacuum, vacuum bagging does not.

Prepreg is produced in a way that there is not much air inside the resin itself. The vacuum will not degas the resin, but it helps to get air out of the system. The pressure inside the autoclave is for the last percents of performance. Out of autoclave prepreg works too, just not quite as good as regular prepreg in an autoclave.

Right, for infusion and prepreg the better the vacuum the better. For wet layup, not so important. Got it.

oekmont
oekmont
Supreme Being (8K reputation)Supreme Being (8K reputation)Supreme Being (8K reputation)Supreme Being (8K reputation)Supreme Being (8K reputation)Supreme Being (8K reputation)Supreme Being (8K reputation)Supreme Being (8K reputation)Supreme Being (8K reputation)
Group: Forum Members
Posts: 550, Visits: 27K
When you do infusion, full vacuum is important. Otherwise there would be trapped air in every corner, because the resin would overflow the corner, leaving behind a cavity of 50% pressurised air. During the process the cavity will shrink down to half it's size while it reaches atmospheric pressure. Accordingly a 100% vacuum cavity shrinks down to zero size.
And you should remember that rotary vane pumps were not invented for composite use only, especially not for vacuum bagging. Many applications require a high vacuum, vacuum bagging does not.

Prepreg is produced in a way that there is not much air inside the resin itself. The vacuum will not degas the resin, but it helps to get air out of the system. The pressure inside the autoclave is for the last percents of performance. Out of autoclave prepreg works too, just not quite as good as regular prepreg in an autoclave.

Steve Broad
Steve Broad
Supreme Being (5.3K reputation)Supreme Being (5.3K reputation)Supreme Being (5.3K reputation)Supreme Being (5.3K reputation)Supreme Being (5.3K reputation)Supreme Being (5.3K reputation)Supreme Being (5.3K reputation)Supreme Being (5.3K reputation)Supreme Being (5.3K reputation)
Group: Forum Members
Posts: 408, Visits: 4.1K
oekmont - 6/12/2020 8:01:13 AM
Theoretically this is 100% true. In most practical hobbyist applications vacuum is applied to keep the carbon cloth in the edges of the mould during cure and that's it. If if you apply 50% vacuum (wich I recommend) it will already remove almost all excess resin. The coth will be pressed together untill the vacuum force equals the force the cloth creates because of fibre stiffness (measure the cloth carefully with a caliper, then again, but press the caliper hard together. There will be a small difference). The resin itself can't create forces to withstand the vacuum while it's liquid, that is the physical definition of a liquid. 100% vacuum will only press the fibres a little bit more together, wich will result in a slightly higher fibre content.
There is nothing like sucking out to much resin. If there is already no pressure in the resin, there is no force wich will move the resin out of the laminate. What really happens is that you degas the resin inside your laminate if you apply too much vacuum. And since there is no movement in the resin, the air can't escape the laminate and will accumulate at the fibre crossings.
If you degas resin in a clear view chamber, you will see that almost nothing happens until you reach about 90% vacuum. But after that an air volume many times that of the resin will be released. Under vacuum pressure, but in case of vacuum bagging the resin will cure that way.

Then why do EC proclaim that their EC.4 pump reaches 99.98% vacuum and autoclaves add even more pressure, if this isn't that important?

Edited 6 Years Ago by Steve Broad
oekmont
oekmont
Supreme Being (8K reputation)Supreme Being (8K reputation)Supreme Being (8K reputation)Supreme Being (8K reputation)Supreme Being (8K reputation)Supreme Being (8K reputation)Supreme Being (8K reputation)Supreme Being (8K reputation)Supreme Being (8K reputation)
Group: Forum Members
Posts: 550, Visits: 27K
Theoretically this is 100% true. In most practical hobbyist applications vacuum is applied to keep the carbon cloth in the edges of the mould during cure and that's it. If if you apply 50% vacuum (wich I recommend) it will already remove almost all excess resin. The coth will be pressed together untill the vacuum force equals the force the cloth creates because of fibre stiffness (measure the cloth carefully with a caliper, then again, but press the caliper hard together. There will be a small difference). The resin itself can't create forces to withstand the vacuum while it's liquid, that is the physical definition of a liquid. 100% vacuum will only press the fibres a little bit more together, wich will result in a slightly higher fibre content.
There is nothing like sucking out to much resin. If there is already no pressure in the resin, there is no force wich will move the resin out of the laminate. What really happens is that you degas the resin inside your laminate if you apply too much vacuum. And since there is no movement in the resin, the air can't escape the laminate and will accumulate at the fibre crossings.
If you degas resin in a clear view chamber, you will see that almost nothing happens until you reach about 90% vacuum. But after that an air volume many times that of the resin will be released. Under vacuum pressure, but in case of vacuum bagging the resin will cure that way.

taimur
t
Supreme Being (484 reputation)Supreme Being (484 reputation)Supreme Being (484 reputation)Supreme Being (484 reputation)Supreme Being (484 reputation)Supreme Being (484 reputation)Supreme Being (484 reputation)Supreme Being (484 reputation)Supreme Being (484 reputation)
Group: Forum Members
Posts: 32, Visits: 122
Vacuum bagging is a technique employed to create mechanical pressure on a laminate during its cure cycle. Pressurizing a composite lamination serves several functions. First, it removes trapped air between layers. Second, it compacts the fiber layers for efficient force transmission among fiber bundles and prevents shifting of fiber orientation during cure. Third, it reduces humidity. Finally, and most important, the vacuum bagging technique optimizes the fiber-to-resin ratio in the composite part. These advantages have for years enabled aerospace and racing industries to maximize the physical properties of advanced composite materials such as carbon, aramid, and epoxy.
What is Fiber-To-Resin Maximization and Why Is It Important?
The reason that composites are used increasingly is the strength-to-weight advantages that they offer. The key to obtaining these advantages is maximizing the fiber-to-resin ratio. The reinforcement (fiberglass, aramid Kevlar®, carbon, etc. is not particularly strong in the textile state. Also, thermosetting resins such as polyester and epoxy are quite brittle if cured without reinforcement. If excess resin exists in the laminate, the laminate will have more of the properties of resin only. If too little resin exists, places where the reinforcement is dry will cause weak spots. To optimize the resin content, the entire reinforcement must be saturated with resin with as little excess as possible. The technique of "squeezing out" excess resin to obtain a maximized fiber-to-resin content is the theory of vacuum bagging.

Steve Broad
Steve Broad
Supreme Being (5.3K reputation)Supreme Being (5.3K reputation)Supreme Being (5.3K reputation)Supreme Being (5.3K reputation)Supreme Being (5.3K reputation)Supreme Being (5.3K reputation)Supreme Being (5.3K reputation)Supreme Being (5.3K reputation)Supreme Being (5.3K reputation)
Group: Forum Members
Posts: 408, Visits: 4.1K
dilligaf76 - 6/2/2020 5:03:29 PM
Chris Rogers - 6/2/2020 2:59:51 PM
I don't totally agree with Steve on the vacuum level - especially if you are doing thin-skinned parts or trying to do core in one shot.  Its one of those things where there are lots of variables and one person's successful recipe of material and process won't translate if you change materials, resin viscosity or layup method.  Mold surface and release system matter too when comparing surface finish outcomes.  I have seen many cases of over-bleed or over-compaction with too much vacuum in wet-layup.  If you are trying to make parts against a mold, 15-20 inHg or about 1/2 the potential vacuum should be fine.  For secondary bonding or thicker parts (2mm+), full vacuum should be fine - and actually preferable.  Make sure the mold you are vacuum-bagging to is fully air-tight or you will have problems.  Envelope bagging is a good idea for small stuff.  Also make sure there is enough resin in your surface layer if you are looking for a cosmetic finish.  And rolling with a bubble-popper is a good idea.

With core, the possibility of pulling resin out of the bottom skin if you are pulling too much vacuum is very real.  Core edges should be well tapered too.

For cosmetic parts (carbon) - doing a wet-preg method with wet-out on plastic can give very good results.  Here's a simple example in a video I made:  

https://youtu.be/06-0Vxs_9nY

This method is extra helpful when you have patterns and slip-joints - which you should totally have for a more complex shape.  

Thank you Chris you seem to know what you're talking about and have educated me a little more than to what I already know, a massive help and appreciate all the comments on here from everyone...

As I mentioned twice, IMO :-) I can only comment on my experience and Chris is quite right that this is a movable feast :-) The only way to find out is to experiment with the method and materials you plan to use. my floor was two layers of carbon, 1/8" core and two more layers of carbon. Full vacuum worked fine for me on this job and many others. A lower vacuum will certainly reduce the risk of defects but will add weight and reduce compaction, but if these aren't a concern then not a problem using a lower vacuum. Only one way to find out..... :-)



dilligaf76
dilligaf76
Supreme Being (760 reputation)Supreme Being (760 reputation)Supreme Being (760 reputation)Supreme Being (760 reputation)Supreme Being (760 reputation)Supreme Being (760 reputation)Supreme Being (760 reputation)Supreme Being (760 reputation)Supreme Being (760 reputation)
Group: Forum Members
Posts: 49, Visits: 115
Chris Rogers - 6/2/2020 2:59:51 PM
I don't totally agree with Steve on the vacuum level - especially if you are doing thin-skinned parts or trying to do core in one shot.  Its one of those things where there are lots of variables and one person's successful recipe of material and process won't translate if you change materials, resin viscosity or layup method.  Mold surface and release system matter too when comparing surface finish outcomes.  I have seen many cases of over-bleed or over-compaction with too much vacuum in wet-layup.  If you are trying to make parts against a mold, 15-20 inHg or about 1/2 the potential vacuum should be fine.  For secondary bonding or thicker parts (2mm+), full vacuum should be fine - and actually preferable.  Make sure the mold you are vacuum-bagging to is fully air-tight or you will have problems.  Envelope bagging is a good idea for small stuff.  Also make sure there is enough resin in your surface layer if you are looking for a cosmetic finish.  And rolling with a bubble-popper is a good idea.

With core, the possibility of pulling resin out of the bottom skin if you are pulling too much vacuum is very real.  Core edges should be well tapered too.

For cosmetic parts (carbon) - doing a wet-preg method with wet-out on plastic can give very good results.  Here's a simple example in a video I made:  

https://youtu.be/06-0Vxs_9nY

This method is extra helpful when you have patterns and slip-joints - which you should totally have for a more complex shape.  

Thank you Chris you seem to know what you're talking about and have educated me a little more than to what I already know, a massive help and appreciate all the comments on here from everyone...

Chris Rogers
C
Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)
Group: Forum Members
Posts: 120, Visits: 933
I don't totally agree with Steve on the vacuum level - especially if you are doing thin-skinned parts or trying to do core in one shot.  Its one of those things where there are lots of variables and one person's successful recipe of material and process won't translate if you change materials, resin viscosity or layup method.  Mold surface and release system matter too when comparing surface finish outcomes.  I have seen many cases of over-bleed or over-compaction with too much vacuum in wet-layup.  If you are trying to make parts against a mold, 15-20 inHg or about 1/2 the potential vacuum should be fine.  For secondary bonding or thicker parts (2mm+), full vacuum should be fine - and actually preferable.  Make sure the mold you are vacuum-bagging to is fully air-tight or you will have problems.  Envelope bagging is a good idea for small stuff.  Also make sure there is enough resin in your surface layer if you are looking for a cosmetic finish.  And rolling with a bubble-popper is a good idea.

With core, the possibility of pulling resin out of the bottom skin if you are pulling too much vacuum is very real.  Core edges should be well tapered too.

For cosmetic parts (carbon) - doing a wet-preg method with wet-out on plastic can give very good results.  Here's a simple example in a video I made:  

https://youtu.be/06-0Vxs_9nY

This method is extra helpful when you have patterns and slip-joints - which you should totally have for a more complex shape.  




Steve Broad
Steve Broad
Supreme Being (5.3K reputation)Supreme Being (5.3K reputation)Supreme Being (5.3K reputation)Supreme Being (5.3K reputation)Supreme Being (5.3K reputation)Supreme Being (5.3K reputation)Supreme Being (5.3K reputation)Supreme Being (5.3K reputation)Supreme Being (5.3K reputation)
Group: Forum Members
Posts: 408, Visits: 4.1K
dilligaf76 - 6/2/2020 1:07:59 PM
Steve Broad - 6/2/2020 9:56:38 AM
dilligaf76 - 6/2/2020 9:31:08 AM
Hi, can anyone tell me what the required Vacuum pressure is required for wet laying Carbon Fibre?

As much as you can manage, IMO. The better the vacuum the better the compaction and carbon/resin ratio. Extreme vacuums are not essential when wet laying, again IMO, but if your vacuum pump can manage 99.95% that will be good.

I've heard that could draw out to much resin and be too dry and cause pin holes etc...
I used peel ply, perforated release film, two layers of breather cloth and the full vacuum capabilities of the EC pump (99.97%) and had no problems. By weight my carbon to resin ratio was between 100:45 and 100:50 with no visible dry patches, pin hoes or delamination.  Image shows car floor under vacuum, showing the resin seeping into the breather cloth having been sucked through the peel ply and release film,



dilligaf76
dilligaf76
Supreme Being (760 reputation)Supreme Being (760 reputation)Supreme Being (760 reputation)Supreme Being (760 reputation)Supreme Being (760 reputation)Supreme Being (760 reputation)Supreme Being (760 reputation)Supreme Being (760 reputation)Supreme Being (760 reputation)
Group: Forum Members
Posts: 49, Visits: 115
Steve Broad - 6/2/2020 9:56:38 AM
dilligaf76 - 6/2/2020 9:31:08 AM
Hi, can anyone tell me what the required Vacuum pressure is required for wet laying Carbon Fibre?

As much as you can manage, IMO. The better the vacuum the better the compaction and carbon/resin ratio. Extreme vacuums are not essential when wet laying, again IMO, but if your vacuum pump can manage 99.95% that will be good.

I've heard that could draw out to much resin and be too dry and cause pin holes etc...

GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search