Group: Forum Members
Posts: 51,
Visits: 707
|
I’d consider a resin brake next time. From the resin line to the back edge use flow media, then from the back edge of the laminate to the vacuum line have a solid 3 fo 4 inch peel ply only layer. This will slow the resin down, allow residual gas to come to the surface and escape, and prevent resin from making it to your vacuum line before all your fibers are infused.