UniMould Gelcoat dont cure


Author
Message
Dokomo
Dokomo
Forum Guru (63 reputation)Forum Guru (63 reputation)Forum Guru (63 reputation)Forum Guru (63 reputation)Forum Guru (63 reputation)Forum Guru (63 reputation)Forum Guru (63 reputation)Forum Guru (63 reputation)Forum Guru (63 reputation)
Group: Forum Members
Posts: 5, Visits: 30
Hi to all. 

It's my first mould using UniMould system. I follow exactly the tutorials and indications for making the mould. 

For the first step, i have bougth locally an MEKP catalyst ( i have attached the image ). I have applied a thin layer of gelcoat, and 4 hours later, another layer. After that, i have wait to the next day to let it cure, but the surprise was, that the part was totally ruined when i arrived next morning ( i have attached another image ). At that time, it had been drying for about 15h.

The gelcoat has reacted with my part ( a motorcycle fuel tank ), producing great wrinkes all around the part. The tank was just finished, laquered and polished with PPG clear coat, and it has been drying for a week before I apply the gelcoat.

The room temperature was about 17º in the day, and about 13º overnight. 

I have made a test yesterday, using 3 small mixes, one in 2%, another in 5% and a extreme one at 10%. The 2% mix, seems to never cure, it has been applied for about 20h right now, and keeps almost fresh. 5% looks nice, it's tacky in the surface and cured in the inside part, and the 10% mix its fully cured.

I think the problem has been that the mixture at 2%, has react because it has been applied over the clear coat too much time without cure ( i look at it 6h after the application and it has no wrinkles at all ), producing the wrinkles at the end.

The question is, it's safe to work at 5% ? Do you think that the problem it's another one ?

Thanks in advance, and sorry about my english. 
Attachments
IMG_20141118_123600.jpg (642 views, 82.00 KB)
IMG_20141118_132727.jpg (620 views, 34.00 KB)
Reply
Dravis
Dravis
Supreme Being (5.1K reputation)Supreme Being (5.1K reputation)Supreme Being (5.1K reputation)Supreme Being (5.1K reputation)Supreme Being (5.1K reputation)Supreme Being (5.1K reputation)Supreme Being (5.1K reputation)Supreme Being (5.1K reputation)Supreme Being (5.1K reputation)
Group: Forum Members
Posts: 592, Visits: 1.9K
According to my old books from my time building glass-fibre/polyester boat hulls, the actual content of MEKP itself in the "catalysts" can vary from 40% and up to 80%

Since the MEKP is just a catalyst, the percentage of catalyst to resin is not very critical, but a combination of only half the expected "actual" percentage of MEKP catalyst AND temperatures that are really a bit too low, and the problem will show its ugly alligatored face ...Crazy

"Sapere Aude"... Dare to KNOW!

The written word is the only truly efficient vehicle for transmitting a complex concept from mind to mind...

103% of all people do not understand statistics...

Do not adjust our mind, theres a fault in reality :-)
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Threaded View
Threaded View
Dokomo - 11 Years Ago
thorstengsxr - 11 Years Ago
Shaneer22 - 11 Years Ago
Dravis - 11 Years Ago
Dokomo - 11 Years Ago
Warren (Staff) - 11 Years Ago
Dokomo - 11 Years Ago
Dokomo - 11 Years Ago
brainfart - 11 Years Ago
Dokomo - 11 Years Ago
matthieutje65 - 11 Years Ago
Dravis - 11 Years Ago
Matt (Staff) - 11 Years Ago

Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search