Group: Forum Members
Posts: 6,
Visits: 231
|
5 layers of 200gsm will give you a solid enough repair. Scarf back damaged tube, I have filled with a piece of styrene foam (closed cell foam is better) if tube shape is compromised, it will give you something to lay up onto. Use the ud, 0*,+30*, 0*, -30*, 0* or a variation of above would work fine. Be careful with your vacuum that you don't crush the foam. You may need to do it in a couple of goes to get the aesthetics right. Jump in and see where it takes you.
|